ASTM A240 S32205 charpy impact tests shall be conducted in accordance with Test Methods and Definitions A 370. Number of Tests—One impact test (3 specimens) shall be made from one plate per heat treatment lot in the final heat treated condition.
ASTM A240 S32205 chemical composition
Grade |
C |
Mn |
P |
S |
Si |
Cr |
Ni |
Mo |
N |
A240 S32205 |
0.03 |
2.00 |
0.030 |
0.02 |
1.0 |
22.0-23.0 |
4.5- |
3.0-3.5 |
0.14-0.20 |
ASTM A240 S32205 mechanical properties
Grade |
Tensile strength, min Mpa |
Yield strength, min Mpa |
Elongation in 2 in % |
Hardness, max |
|
Brinell |
Rockwell B |
||||
A240 S32205 |
655 |
450 |
25 |
293 |
31 |
ASTM A240 S32205 Orientation of Test Specimens--Unless specified as transverse specimens (long axis of the specimen transverse to the final rolling direction, root of the notch perpendicular to the rolling face) on the purchase order, the orientation of the specimens shall be longitudinal (long axis of the specimen parallel to the final rolling direction, root of the notch perpen- dicular to the rolling face). The manufacturer is permitted to test transverse specimens provided that such tests meet the acceptance criteria applicable to longitudinal specimens. Un- less otherwise specified on the purchase order, the specimens shall be taken so as to include the mid-thickness of the product.