P355NH, P355NL1, P355NL2 boiler steel what are the tensile requirements?

P355NH steel is used by the world's fabricators for the manufacture of pressure vessel tanks for the storage of pressurized gases. P355NL1 steel is ideal for use in low temperatures. Grade P355NL2 is ideal for use in especially low temperatures.

P355NH, P355NL1, P355NL2 boiler steel composition

 

P355NH

P355NL1

P355NL2

C

0.18

0.16

0.16

Si

0.50

0.40

0.40

Mn

1.10 to 1.70

0.80 to 1.50

0.80 to 1.50

P

0.025

0.025

0.020

S

0.015

0.015

0.010

Al

0.020

0.020

0.020

N

0.012

0.012

0.012

Cr

0.30

0.30

0.30

Cu

0.30

0.30

0.30

Mo

0.08

0.08

0.08

Nb

0.05

0.05

0.05

Ni

0.50

0.50

0.50

Ti

0.03

0.03

0.03

V

0.05

0.05

0.05

P355NH, P355NL1, P355NL2 boiler steel tensile requirements


Grade

Type

Thickness (mm)

Yield strength
mpa (min)

Tensile strength
mpa

Elongation
% (min)

P355NH

Normalized

≤ 16

355

490 - 630

21

P355NL1

 

16> to ≤40

345

490 - 630

21

P355NL2

 

40> to ≤60

335

490 - 630

21

 

 

60> to ≤100

315

470 - 610

21

 

 

100> to ≤150

305

460 - 600

21

 

 

150> to ≤250

295

450 - 590

21

(Please note: the technical information above is for guidance only – for exact specifications please check with our Sales Team)
P355NH, P355NL1, P355NL2 boiler steel plates are hot selling in our company.