35crmo steel Heat treatment


35CrMo alloy steel tube with hollow section, a large number of pipelines used for conveying fluids, such as oil, natural gas, gas, water and some solid materials pipelines. The 35CrMo alloy steel working temperature is up to 500 ° C, the low temperature can be -100 ° C, and has high static strength and high fatigue strength, good hardenability, no tendency to overheat, small quenching deformation, and moderate machinability.

35CrMo alloy steel Chemical Composition [%]

Grade

C

Si

Mn

Cr

Mo

V

35CrMo

0.32-
0.40

0.17-
0.37

0.40-
0.70

0.80-
1.10

0.15-
0.25

-

35CrMo Alloy Steel Mechanical Properties

Yield strength: ≥ 835 MPa
Tensile strength: ≥ 980 MPa
Elongation: ≥12%
Rate of reduction in area: ≥45%
Impact absorbing energy: ≥ 63 J
Brinell Hardness: ≤ 229 (Annealed or high temperature tempered steel rod)
Sample size: 25mm

Heat treatment specification:

First quenching heating temperature: 850 °C (Coolant – oil)
Tempering heating temperature: 600 °C (Coolant – water, oil)